Processing Machinery 7 visualizaciones

PVDF Product Sink Marks

Fenómeno del problema
Depressed sink marks at thick-walled areas.
Análisis de la causa
PVDF has high crystallinity and a relatively large shrinkage (about 2~3%); insufficient shrinkage compensation in thick areas forms depressions.; During on-site troubleshooting, verify item by item according to this mechanism, and avoid blindly adjusting the machine based solely on experience
Solución
①Increase holding pressure and time; ②core out thick areas to even the wall thickness; ③enlarge the gate to delay freeze-off; ④optimize the holding pressure curve.; After adjustment, take consecutive samples to verify the effect, and resume mass production only after confirming stability
Conclusión clave
PVDF's high shrinkage makes sink mark management important; holding pressure and structural design are equally emphasized.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PVDF;sink marks;shrinkage;holding pressure;wall thickness;coring out