Processing Machinery 7 visualizaciones

SMMA Processing Temperature Too High

Fenómeno del problema
SMMA products yellow, degrade and have silver streaks, with barrel temperature exceeding 230℃ or residence timeout at 260℃.
Análisis de la causa
SMMA barrel temperature upper limit 230℃; residence at 260℃ not exceeding 5-6 minutes; over-temperature or over-time thermal degradation; yellowing and performance decline; transparency loss.
Solución
①Barrel temperature ≤230℃; ②residence at 260℃ ≤5-6 minutes; ③optimize cycle to shorten residence; ④purge the machine after degradation.; after adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability
Conclusión clave
SMMA's 230℃ upper limit and 5-6 minute residence are the degradation defense line; cycle management is prevention; purging keeps purity.; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
SMMA;temperature;230℃;degradation;residence;yellowing

¿Le ha resultado útil?

0 personas encontraron esto útil