Material Drying 8 visualizaciones

EEA injection thick-wall bubbles

Fenómeno del problema
Dense bubbles of 0.1-0.5mm appearing inside EEA injection molded thick-wall products, concentrated in the wall thickness center
Análisis de la causa
Holding pressure insufficient <40MPa or holding time short, thick-wall center not compacted; raw material contains moisture; injection speed too fast entrapping air; poor mold venting
Solución
1) Increase holding pressure to 60-80MPa; 2) Extend holding time to fully compact the thick wall; 3) Fully dry the raw material to moisture <0.02%; 4) Add vent grooves or vent pins to the mold; 5) Gradually decelerate injection to avoid air entrapment
Conclusión clave
Thick-wall bubbles are caused by a combination of insufficient holding, moisture and poor venting
EEA injectionbubblesholding pressurethick-wall productmold venting

¿Le ha resultado útil?

0 personas encontraron esto útil

ChemAI