Material Drying 8 visualizaciones

EMA Processing Moisture Causes Silver Streaks

Fenómeno del problema
White silver streaks appear on the surface of EMA injection molded products
Análisis de la causa
Raw material contains moisture >0.05%, which vaporizes during high-temperature processing to form bubbles that are stretched into silver streaks; insufficient drying or condensed water vapor in the hopper
Solución
1) Dry the raw material at 80°C for 3-4h to moisture <0.02%; 2) Increase back pressure 0.5-1MPa for venting; 3) Reduce injection speed to avoid air entrapment; 4) Heat the hopper to prevent condensed water vapor
Conclusión clave
Silver streaks are caused by moisture vaporization and stretching; drying and venting are the main countermeasures
EMA injection silver streaks moisture drying venting back pressure