Injection Molding 7 visualizaciones

EVOH injection flash is severe

Fenómeno del problema
EVOH injection molded product parting line flash 0.05-0.1mm, width >2mm, requiring secondary trimming
Análisis de la causa
Injection pressure too high >80MPa with melt overflowing from the parting line; insufficient clamping force; mold parting line fit gap >0.02mm
Solución
1) Reduce injection pressure to 60-70MPa; 2) Increase clamping force or use a larger tonnage '2079851475616104452 machine; 3) Mold fit gap <0.02mm; 4) Increase melt viscosity to reduce mold penetration tendency
Conclusión clave
Flash is caused by high-pressure injection and mold gap; reducing pressure and improving mold fit are key
EVOH injection flash clamping force parting line injection pressure

¿Le ha resultado útil?

0 personas encontraron esto útil