Injection Molding
15 visualizaciones
Burning from poor venting in PET preform '2079851475616104452
Fenómeno del problema
Burn marks or black spots appear at the PET preform end (far from the gate), accompanied by irritating odor.
Análisis de la causa
Poor cavity venting; air rapidly compressed producing high temperature (diesel effect) causing local burning, vent grooves blocked or injection too fast.
Solución
Deepen and widen vent grooves (0.02-0.04mm); clean accumulated material; appropriately reduce injection speed; optimize gate position.
Conclusión clave
PET preform burning is the result of air not being able to escape in time; improving venting is fundamental.
¿Le ha resultado útil?
0 personas encontraron esto útil
¡Gracias por sus comentarios!