Injection Molding
3 조회수
Low weld line strength in EEA injection
문제 현상
Strength of EEA injection molded multi-gate products at the weld line is only 30-40% of the whole
원인 분석
The temperature of the two melt fronts has dropped, causing small molecular chain diffusion depth and insufficient entanglement; dispersed phase orientation discontinuous at the weld line
해결 방법
1) Increase injection temperature by 10-15°C to increase diffusion depth; 2) Increase injection speed to keep the front temperature higher; 3) Increase holding pressure to ensure compaction at the weld; 4) Set an overflow well at the weld line and remove it afterwards
핵심 요약
Low weld line strength is caused by insufficient molecular entanglement; high-temperature high-speed injection and overflow wells are effective countermeasures
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!