Injection Molding 6 visualizações

Low weld line strength in EEA injection

Fenómeno do problema
Strength of EEA injection molded multi-gate products at the weld line is only 30-40% of the whole
Análise das causas
The temperature of the two melt fronts has dropped, causing small molecular chain diffusion depth and insufficient entanglement; dispersed phase orientation discontinuous at the weld line
Solução
1) Increase injection temperature by 10-15°C to increase diffusion depth; 2) Increase injection speed to keep the front temperature higher; 3) Increase holding pressure to ensure compaction at the weld; 4) Set an overflow well at the weld line and remove it afterwards
Conclusão principal
Low weld line strength is caused by insufficient molecular entanglement; high-temperature high-speed injection and overflow wells are effective countermeasures
EEA injectionweld lineinsufficient entanglementinjection temperatureoverflow well