Material Analysis 12 조회수

EVOH heat-sensitive degradation and discoloration

문제 현상
EVOH processing >230°C turns yellow-brown with decreased mechanics
원인 분석
EVOH vinyl alcohol groups decompose by dealcoholization at high temperature, starting >230°C; excessive residence time aggravates decomposition
해결 방법
1) Strictly control the upper limit of processing temperature at 190-230°C; 2) Shorten high-temperature residence and increase rotation speed; 3) Add 0.1wt% heat stabilizer; 4) Select low vinyl alcohol content EVOH (ethylene 32-38%) with low decomposition tendency
핵심 요약
EVOH heat-sensitive decomposition is caused by vinyl alcohol dealcoholization; temperature control is the fundamental countermeasure
EVOH thermal decomposition dealcoholization yellowing heat stabilizer temperature control