Injection Molding
3 조회수
CEF internal stress concentration severe
문제 현상
The internal stress of the CEF product is >15MPa, causing cracking during storage
원인 분석
The injection speed is too fast and the orientation stress is large; uneven cooling freezes thermal stress; the gate position is improper and the flow orientation is concentrated
해결 방법
1) Reduce the injection speed to reduce orientation; 2) Uniform mold temperature to reduce thermal stress; 3) Anneal at 80°C/4h to release stress; 4) Optimize the gate position
핵심 요약
Internal stress is caused by fast injection and uneven cooling; reducing speed, uniform cooling and annealing are the key
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다