Extrusion & Post
4 조회수
Cracks on the Surface of acrylonitrile-styrene-acrylate copolymer Extruded Profiles
문제 현상
Cracks appear on the surface of the extruded profiles, affecting the product appearance and subsequent processing quality.
This problem is common in acrylonitrile-styrene-acrylate copolymer extrusion production.
원인 분석
(1)The extrusion temperature (220-260°C) is set improperly, and the melt quality is unstable
(2)The screw rotation speed and the haul-off speed are improperly matched
(3)Die condition or design problems
(4)The cooling system is set improperly
(5)Raw material quality or pretreatment problems
해결 방법
(1)Optimize the extrusion temperature to a reasonable value within the 220-260°C range
(2)Stabilize the screw rotation speed and the haul-off speed
(3)Check the die condition, clean the accumulated material or repair the damage
(4)Adjust the cooling water temperature and flow
(5)Ensure the raw material is dried (70-80°C, 3-4h) and clean
핵심 요약
Extrusion surface defects need to be controlled from three aspects: temperature, speed, and die condition.
이 정보가 도움이 되었나요?
0 명이 도움이 되었다고 합니다
의견 주셔서 감사합니다!