Extrusion & Post 10 조회수

PEEK 3D printing poor interlayer bonding force

문제 현상
3D printed parts delaminate between layers, with extremely low Z-direction strength
원인 분석
The previous layer has fully cooled and crystallized, unable to achieve effective diffusion and entanglement with subsequent layers; the printing chamber temperature is insufficient to maintain the interface temperature
해결 방법
Increase the printing chamber temperature to above 140°C (even close to Tg=143°C) to keep the interlayer in a semi-molten state; reduce the layer thickness (such as 0.1mm) to increase heat penetration; overall annealing after printing
핵심 요약
Interlayer bonding is the core technical difficulty of PEEK additive manufacturing
3D printinginterlayer bonding forcechamber temperatureannealingadditive manufacturing