Molds & Tooling 1 views

POM sink marks and voids

Problem Phenomenon
Surface depressions at thick walls or internal voids.
Cause Analysis
POM has large volume shrinkage; after the gate freezes, feeding to the thick-walled core is interrupted; holding pressure transmission is insufficient.
Solution
①Conduct a gate freeze study to determine holding time; ②enlarge the gate; ③reduce material in thick walls; ④increase holding pressure.
Key Takeaway
POM feeding = gate freeze time management.
POM;sink marks;voids;gate freeze;holding pressure