Processing Machinery 1 views

PVC Processing Window 160-195℃

Problem Phenomenon
PVC products yellow and discolor, degradation signs appear when barrel temperature is slightly high, process adjustment space extremely small
Cause Analysis
PVC is the general-purpose plastic with the worst thermal stability, processing window only 160-195℃, absolute upper limit 200℃; exceeding it starts the de-HCl degradation chain reaction, temperature tolerance only ±5-10℃
Solution
①Melt temperature rigid 175-195℃, soft 160-180℃; ②Absolutely not exceeding 200℃; ③Temperature control precision ±3℃ and regularly calibrate thermocouples
Key Takeaway
PVC temperature discipline is the strictest among general-purpose plastics; 200℃ is an untouchable red line, the narrow window determines dual high requirements for equipment and management; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PVC; processing window; 160-195℃; 200℃; temperature control