Processing Machinery 1 views

PVDF Melt Temperature Degradation

Problem Phenomenon
The product discolors and turns yellow, produces black specks, accompanied by a pungent odor.
Cause Analysis
PVDF begins thermal decomposition and releases HF when the processing temperature exceeds about 300℃; loss of temperature control or excessive residence accelerates decomposition.; During on-site troubleshooting, verify item by item according to this mechanism, and avoid blindly adjusting the machine based solely on experience
Solution
①Control the melt temperature within the 230~290℃ window; ②strictly prohibit exceeding 300℃; ③shorten the residence time; ④immediately lower the temperature, clean the machine, and ventilate after decomposition.
Key Takeaway
PVDF thermal decomposition releasing HF poses both quality and safety risks; 300℃ is an insurmountable red line.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PVDF;degradation;discoloration;hydrofluoric acid;temperature;decomposition