PPSU insufficient drying produces bubbles

Problem Phenomenon
During PPSU processing, bubbles and silver streaks appear in products.
Cause Analysis
PPSU has relatively strong hygroscopicity (water absorption 0.6%); with insufficient drying, moisture vaporizes and explodes at the ultra-high processing temperature of 340-390°C to form bubbles.
Solution
Dry at 135-150°C for 4-6h to moisture <0.03%, dew point ≤-35°C.
Key Takeaway
PPSU super drying is a basic processing requirement.