Injection Molding 7 visualizações

ASA Glass Fiber Exposure Floating Fiber

Fenómeno do problema
【Problem Phenomenon】Glass fiber reinforced ASA surface fibers exposed and rough
Análise das causas
Fibers enrich the surface with melt flow; when melt temperature and mold temperature are low and injection speed slow, fibers are difficult to be coated by resin; during on-site troubleshooting, verify item by item according to this mechanism, avoid blindly adjusting the machine based only on experience
Solução
Increase melt temperature and mold temperature to improve coating; increase injection speed to embed fibers; mold polishing reduces fiber retention; after adjustment, continuously sample to verify the effect, and resume mass production after confirming stability
Conclusão principal
ASA floating fibers suppressed by temperature and injection speed, mold polishing assists; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence; include this case in the defect archive as a troubleshooting reference for subsequent similar problems
floating fiber glass fiber coating injection speed