PA66 over-drying embrittlement

Fenómeno do problema
After pellet moisture content is reduced too low, product brittleness increases instead, impact test unqualified
Análise das causas
Over-drying (over 110℃ or over 12 hours) causes thermal oxidation, PA66 pellets yellow, impact and elongation at break decline; recycled material has higher risk due to accumulated heat history
Solução
①Control moisture content in the 0.1-0.2% range, do not blindly pursue lower; ②if not put into production after 8 hours, lower to 70-80℃ for heat preservation; ③shorten drying time for recycled material and strengthen verification
Conclusão principal
PA66 drying has over-drying risk; 0.1-0.2% is the target range, overtime heat preservation with temperature reduction is the standard handling for production handover; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence