Material Drying 10 visualizações

PA66 extruded rods and plates

Fenómeno do problema
Extruded PA66 rods have center bubbles and surface ripples, and internal looseness after machining
Análise das causas
Rods have large wall thickness, the outer layer cools first and center feeding is insufficient, forming shrinkage voids and bubbles; micro-bubbles from insufficient drying also remain in the center; extrusion temperature fluctuation causes surface ripples; during on-site troubleshooting, verify item by item according to this mechanism, avoiding blindly adjusting the machine based only on experience
Solução
①Fully dry the raw material to moisture content ≤0.15%; ②Sizing sleeve slow cooling to reduce inner-outer temperature difference; ③Extrusion temperature stable within ±2℃ fluctuation; after adjustment, take continuous samples to verify the effect, confirm stability before resuming mass production
Conclusão principal
The internal quality of PA66 rods relies on dual control of drying and slow cooling; once center shrinkage voids form they cannot be remedied, prevention is the only means; after confirming effectiveness, fix the parameters and practices into the work instructions to prevent recurrence
PA66;extrusion;rod;shrinkage void;slow cooling

Isto foi útil?

0 pessoas acharam isto útil