Material Drying 6 visualizações

PPO PPX Grade Low-Temperature Process

Fenómeno do problema
【Problem Phenomenon】PPO/PP alloy PPX grades processed according to the high-temperature process show material degradation and discoloration
Análise das causas
NORYL PPX is a PPO/PP alloy, drying 65-75℃×2-4h, mold temperature 40-65℃, melt 260-300℃; the PP component determines its low-temperature process window, and high-temperature processing causes degradation
Solução
Execute PPX with 65-75℃ drying and 40-65℃ mold temperature; melt must not exceed 300℃; purge according to PP procedures; after adjustment, continuously sample to verify the effect, and resume mass production after confirming stability
Conclusão principal
PPX is a PP alloy low-temperature material, 65-75℃ drying and 40-65℃ mold temperature; after confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence