Molds & Tooling 8 visualizações

PPS mold temperature 130-150℃

Fenómeno do problema
Product surface has no gloss and appears matte and rough, warpage after demolding, heat resistance not up to standard
Análise das causas
PPS is a crystalline polymer, mold temperature determines crystallinity: crystallinity at 94℃ mold temperature is only about 8%, reaching 48% at 150℃; mold temperature below 120℃ causes rough and glossless product surface, insufficient crystallization, and post-crystallization deformation
Solução
①Mold temperature standard set at 130-150℃; ②when surface requirements are high it must not be lower than 120℃; ③use oil temperature unit plus insulation plate for precise control; After adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability
Conclusão principal
Mold temperature is the switch of PPS crystallinity; 130-150℃ ensures sufficient crystallization, glossy surface and dimensional stability; After confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
PPS; mold temperature; 130-150℃; crystallinity; gloss