Extrusion & Post 14 visualizações

PVB Improper Extrusion Temperature Degradation

Fenómeno do problema
PVB film shows yellowing, degradation spots, and performance decline, extrusion temperature out of control exceeding 200℃ or long-term high-temperature residence.
Análise das causas
PVB processing temperature is 160~200℃, too high temperature causes thermal degradation; long-term high-temperature residence accumulates heat history; local overheating area degradation; uneven temperature distribution.
Solução
①Control extrusion temperature within 160~200℃; ②Avoid long-term high-temperature residence; ③Temperature distribution uniformity management; ④Purge the machine after degradation.; After adjustment, continuously sample to verify the effect, confirm stability before resuming mass production
Conclusão principal
PVB's 160~200℃ temperature window prevents degradation; residence time management is equally important; uniformity guarantees consistent quality.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence
PVB;temperature;degradation;yellowing;residence;uniformity