Extrusion & Post 13 visualizações

Die buildup and carbon deposits in EAA extrusion

Fenómeno do problema
After EAA extrusion shutdown, a brown carbon deposit layer is found on the inner wall of the die, and black specks appear on the product surface after restarting
Análise das causas
EAA is heated for a long time in the die stagnation zone, oxidized, decomposed and carbonized; the die is not cleaned in time during shutdown; high extrusion temperature accelerates carbonization
Solução
1) Flush the die with pure PE for 3-5min before shutdown to remove EAA residue; 2) Disassemble and clean the die immediately after shutdown; 3) Lower the extrusion temperature by 5-10°C to reduce carbonization tendency; 4) Optimize the die flow channel to reduce stagnation zone dead corners
Conclusão principal
Die carbon deposits are caused by thermal oxidation and untimely cleaning; PE flushing and timely cleaning are the key
EAA extrusion die carbon deposit PE flushing stagnation zone thermal oxidation