Injection Molding 6 visualizações

EEA injection mold venting burnt

Fenómeno do problema
Insufficient venting in EEA injection mold, air in the cavity compressed and heated causing local burnt
Análise das causas
Insufficient vent groove area or improper position; injection speed too fast, air having no time to escape; air compressed to high temperature >200°C causing oxidative burnt
Solução
1) Increase vent groove area, depth 0.02-0.03mm, width 5-10mm; 2) Set vent grooves in the last-fill area of the melt; 3) Reduce injection speed to reduce air compression; 4) Multi-stage injection with slow advancement for venting
Conclusão principal
Burnt is caused by insufficient venting and high-speed injection compressing air; increasing venting and reducing speed is the key
EEA injectionmold burntvent grooveinjection speedair compression

Isto foi útil?

0 pessoas acharam isto útil