EMA Film Excessive Heat Shrinkage
Fenómeno do problema
EMA film heat shrinkage at 80°C >12%, exceeding the 5% dimensional stability requirement
Análise das causas
EMA extrusion orientation releases after heating, causing large shrinkage; EMA thermal expansion coefficient large; film cooling freezes a large amount of orientation stress
Solução
1) Reduce extrusion draw ratio to reduce orientation freezing; 2) Anneal film at 60-80°C to release orientation stress; 3) Add 5-10wt% rigid resin to reduce heat shrinkage; 4) Biaxial stretching process to balance orientation
Conclusão principal
Film heat shrinkage is caused by orientation freezing; reducing draw ratio and annealing treatment are key