Extrusion & Post 13 visualizações

EMA Extruded Film Poor Thickness Uniformity

Fenómeno do problema
EMA extruded film transverse thickness deviation ±15%, exceeding the ±5% industry standard
Análise das causas
Unreasonable die flow channel design causes uneven melt flow in the wide die; EMA melt elasticity large, extrusion swell uneven; air ring cooling uneven
Solução
1) Adopt coat-hanger die design to ensure uniform transverse flow; 2) Fine-tune die gap ±0.02mm; 3) Optimize air ring air volume and angle for uniform cooling; 4) Add a small amount of low-elasticity resin to reduce swell differences
Conclusão principal
Film thickness uniformity needs coordinated optimization from three aspects: die design, gap adjustment and cooling
EMA film thickness uniformity die design extrusion swell air ring cooling