Molding Process
3 visualizações
EVA foam hardness is too high
Fenómeno do problema
EVA foamed shoe sole Shore C50 is higher than C35-40
Análise das causas
Density >0.3 with few cells, thick walls and hardness; crosslinking >80% with insufficient elasticity
Solução
1) Increase AC to 0.8-1wt% to reduce density to 0.25g/cm³; 2) Reduce DCP to 0.4-0.5wt% with crosslinking 60-70%; 3) VA18-28% to reduce viscosity and promote expansion
Conclusão principal
High hardness is caused by high density and excessive crosslinking; reducing density and moderate crosslinking are key