Injection Molding
1 visualizações
EVOH '2079851475616104452 Sink Marks
Fenómeno do problema
EVOH injection molded products show 0.2-0.5mm surface depression sink marks in thick-walled areas
Análise das causas
Insufficient holding pressure or short holding time; gate freezes too early so holding pressure cannot be transmitted; large wall thickness differences, after thin walls freeze the thick walls cannot be fed
Solução
1) Increase holding pressure to 70-90MPa; 2) Extend holding to gate freeze +2s; 3) Product design to reduce wall thickness differences with gradual transitions; 4) Add supplementary gates in thick-walled areas
Conclusão principal
Sink marks are caused by insufficient holding and wall thickness differences; high holding pressure and multiple gates are the core countermeasures