Material Overflow at EVOH Vacuum Vent
Fenómeno do problema
Material overflows at EVOH extrusion vacuum vent, vent hole clogged
Análise das causas
EVOH melt viscosity low, overflowing at vacuum section; vacuum section temperature too high, viscosity even lower, aggravating overflow; vent hole design improper
Solução
1) Reduce vacuum section temperature by 5-10°C to increase viscosity; 2) Add baffle above vent hole to prevent overflow; 3) Increase screw speed to accelerate conveyance and reduce residence
Conclusão principal
Overflow is caused by low melt viscosity; cooling and adding baffle are key