Molding Process
3 visualizações
EVOH Surface Stress Whitening
Fenómeno do problema
Stress whitening on stressed areas of EVOH product surfaces, affecting appearance and strength
Análise das causas
EVOH molecular orientation under local stress causes refractive index difference and whitening; areas of internal stress concentration in the product
Solução
1) Reduce injection speed to decrease orientation stress; 2) Anneal at 80°C/2h to release stress; 3) Product design to avoid stress-concentrating sharp corners
Conclusão principal
Stress whitening is caused by orientation and internal stress; reducing orientation and annealing are key
Isto foi útil?
0 pessoas acharam isto útil