Material Drying
7 visualizações
Silver streaks caused by moisture in PU processing
Fenómeno do problema
White silver streaks appear on the surface of PU injection molded products
Análise das causas
Raw material contains moisture >0.05%, which vaporizes during high-temperature processing to form bubbles that are stretched into silver streaks; insufficient drying or moisture condensation in the hopper
Solução
1) Dry raw material at 80°C for 3-4h to moisture <0.02%; 2) Increase back pressure 0.5-1MPa for venting; 3) Reduce injection speed to avoid air entrapment; 4) Heat the hopper to prevent moisture condensation
Conclusão principal
Silver streaks are caused by moisture vaporization and stretching; drying and venting are the main countermeasures
Isto foi útil?
0 pessoas acharam isto útil
Obrigado pelo seu comentário!