Injection Molding
1 visualizações
Difficult demolding in PVA '2079851475616104452
Fenómeno do problema
PVA injection molded products have large demolding force, products deformed or scratched, demolding time accounts for 30% of the cycle
Análise das causas
Large adhesion between PVA and mold cavity; draft angle insufficient <0.5°; cooling time insufficient, product demolded before fully solidified; ejection mechanism design unreasonable
Solução
1) Increase mold draft angle to 1-2°; 2) Extend cooling time so that the product is fully solidified before demolding; 3) Polish mold surface to Ra<0.2μm; 4) Increase ejection area, use large-area ejector plate; 5) Spray mold release agent (temporary solution)
Conclusão principal
Difficult demolding is caused by adhesion and insufficient mold design; increasing draft angle is the fundamental measure