Injection Molding 6 visualizações

Linear marks appear around multiple gates or holes of the product

Fenómeno do problema
Linear marks appear around multiple gates or holes of the product, strength significantly lower than normal areas, color at the weld line differs from the surroundings
Análise das causas
Before confluence of melt from multiple gates, temperature has dropped, poor fusion Injection speed on the low side, insufficient melt front temperature Insufficient mold venting, gas at the weld hinders fusion Melt flow path too long, large temperature drop Excessive lubricant reducing melt adhesion
Solução
Increase injection speed to keep the melt front at high temperature Appropriately raise barrel temperature to the high side of 170-230°C Add vent grooves or overflow wells at the weld line Shorten the flow path or adjust gate position Reduce lubricant addition
Conclusão principal
Weld lines require increasing confluence temperature, improving venting and optimizing gates
weld linepoor fusioninjection speedventing