Voltar a Problema e solução
Extrusion & Post 13 visualizações

CEF extrusion die hang-up and carbon deposits

Fenómeno do problema
After CEF extrusion shutdown, brown carbon deposit layer found on the die inner wall, black specks on the product surface when restarting
Análise das causas
CEF stays in the die residence area for a long time, heated, oxidized, decomposed and carbonized; die not cleaned in time during shutdown; extrusion temperature too high accelerates carbonization
Solução
1) Flush the die with pure PE for 3-5min before shutdown to remove CEF residue; 2) Disassemble and clean the die immediately after shutdown; 3) Lower the extrusion temperature by 5-10°C to reduce carbonization tendency; 4) Optimize die flow channels to reduce dead spots in residence areas
Conclusão principal
Die carbon deposits are caused by thermal oxidation and untimely cleaning, PE flushing and timely cleaning are key
CEF extrusiondie carbon depositPE flushingresidence areathermal oxidation