Injection Molding 6 visualizações

CEF injection sink marks

Fenómeno do problema
The surface of the thick-walled area of the CEF injection molded part is dented 0.2-0.5mm, sink marks
Análise das causas
The holding pressure is insufficient or the holding pressure time is short; the gate freezes too early and the holding pressure cannot be transmitted; the wall thickness difference is large, and the thick wall cannot be fed after the thin wall freezes
Solução
1) Increase the holding pressure to 70-90MPa; 2) Extend the holding pressure to gate freezing +2s; 3) Product design to reduce wall thickness differences with gradual transition; 4) Add supplementary gates in the thick-walled area
Conclusão principal
Sink marks are caused by insufficient holding pressure and wall thickness differences; high-pressure holding and multiple gates are the core countermeasures
CEF injectionsinkholding pressurewall thickness differencegate design