Material Drying
7 visualizações
DSTDP '2079851475616104452 thick-wall bubbles
Fenómeno do problema
Dense bubbles 0.1-0.5mm appear inside DSTDP injection molded thick-wall products, concentrated in the center of the wall thickness
Análise das causas
Holding pressure insufficient <40MPa or holding time short, thick-wall center not compacted; raw material contains moisture; injection speed too fast entraining air; poor mold venting
Solução
1) Increase holding pressure to 60-80MPa; 2) extend holding time so the thick wall is fully compacted; 3) fully dry raw material to moisture <0.02%; 4) add vent grooves or vent pins to the mold; 5) progressively decelerate injection to avoid air entrainment
Conclusão principal
Thick-wall bubbles are caused by a combination of insufficient holding pressure, moisture and poor venting
Isto foi útil?
0 pessoas acharam isto útil