Fenómeno do problema
Glass Fibre injection molded product gate freezes within 0.5-1s during holding stage, holding pressure cannot be transmitted, product severe sink
Análise das causas
Gate size too small, diameter <1mm causes fast freezing; injection temperature too low; mold temperature too low accelerates gate cooling
Solução
1) Increase gate diameter to 1.5-2mm; 2) raise injection temperature to 160-220°C; 3) raise mold temperature to 40-50°C to delay gate freezing; 4) holding pressure decays in steps rather than sudden release
Conclusão principal
Premature gate freezing is caused by small gate and low temperature; enlarging gate and raising temperature are fundamental measures