POE film printing adhesion poor

Fenómeno do problema
POE film ink adhesion after printing
Análise das causas
POE surface polarity has poor affinity with ink; corona treatment effect decays quickly; ink system does not match POE
Solução
1) Print immediately after corona treatment, within 24h; 2) Use POE-specific ink; 3) Increase corona power to 15-20kW/m² to ensure surface tension >42mN/m; 4) Flame treatment to assist surface polarization
Conclusão principal
Poor printing adhesion is caused by insufficient surface polarity; corona treatment and special ink are key
POE filmprinting adhesioncorona treatmentspecial inksurface tension