Extrusion & Post 7 visualizações

FEP melt fracture

Fenómeno do problema
FEP extruded products show severe surface appearance defects of melt fracture/sharkskin
Análise das causas
FEP has a low critical shear stress (similar to other perfluoropolymers), and the extrusion speed is too high and exceeds the critical value; the die temperature is too low or the design is improper
Solução
Reduce the extrusion line speed to below the critical speed; raise the die temperature (up to 370°C); optimize the die entrance angle to reduce elastic turbulence
Conclusão principal
Melt fracture is a common challenge faced in the extrusion processing of perfluoropolymers