Extrusion & Post 10 visualizações

Metallocene linear low density polyethylene blown film poor transparency

Fenómeno do problema
The film haze is high and transparency does not meet requirements. Poor transparency affects product appearance and display effect, especially important in packaging films and optical films.
Análise das causas
(1) Metallocene linear low density polyethylene has high crystallinity, crystalline regions scatter light causing high haze\ (2) Melt temperature too low, plasticization insufficient\ (3) Cooling rate slow, crystallinity high\ (4) The raw material contains impurities or gel\ (5) Film surface rough
Solução
(1) Appropriately increase the extrusion temperature to the higher value within the 190-260°C range, fully plasticize\ (2) Improve air ring cooling efficiency, speed up cooling to reduce crystallinity\ (3) Select grades with good transparency or add a nucleating agent to refine grains\ (4) Strengthen filtration, use 80-120 mesh filter screen to remove impurities\ (5) Polish the die to improve film surface finish
Conclusão principal
Poor transparency is caused by high crystallinity or impurities, and needs improvement by increasing temperature, speeding up cooling and selecting suitable materials.
poor transparencycrystallinitycooling ratenucleating agenthaze