Poor electroplating adhesion of polystyrene ABS products
Fenómeno do problema
Poor coating adhesion after electroplating of ABS products, prone to blistering or peeling.
ABS is the most commonly used electroplating plastic.
Análise das causas
(1) Unsuitable product surface roughness, affecting roughening effect
(2) Large product internal stress, affecting coating adhesion
(3) Improper processing temperature, uneven material structure
(4) Residual mold release agent affecting electroplating
(5) ABS grade not suitable for electroplating
Solução
(1) Select electroplating-grade ABS grades
(2) Optimize processing temperature within the 180-240°C range, reduce internal stress
(3) Do not use mold release agent or use easy-to-clean type
(4) Product surface annealing treatment (60-80°C, 2h)
(5) Polystyrene controls mold temperature at the higher value within the 40-80°C range
Conclusão principal
ABS electroplating quality is closely related to material grade and internal stress.