Injection Molding 10 visualizações

Insufficient fiber retention length in the product

Fenómeno do problema
Inspection finds that the fiber length in the product is <0.5mm, far below the design target
Análise das causas
The shear in the screw mixing section is too strong, cutting the glass fibers; the shear rate at the runner/gate of the injection system is too high; the material is repeatedly cut through multiple thermal histories
Solução
Use a low-shear screw design (L/D=18-20, compression ratio 1.5-1.8); optimize runner and gate dimensions with smooth transitions to reduce shear rate; reduce screw speed
Conclusão principal
Fiber retention length is the primary factor determining the reinforcement effect