Product burnt spots/yellowing

Fenómeno do problema
Brown burnt spots appear locally on the product or the overall color is yellowish
Análise das causas
The PP matrix undergoes thermo-oxidative degradation at temperatures >230°C; the impregnation treatment agent on the glass fiber surface decomposes at high temperature; the material stays in the barrel too long
Solução
Strictly control the maximum processing temperature ≤240°C; shorten material residence time to <5 minutes; add antioxidant (such as 1010+168 compound system)
Conclusão principal
The LGFPP processing temperature window is narrow, and a balance must be found between plasticization and degradation
burnt spotsyellowingdegradationprocessing temperatureantioxidantresidence time