Extrusion & Post 5 görüntüleme

LDPE Film Sharkskin

Sorun Belirtisi
Periodic ripples like sharkskin appear on the film bubble surface, and the gloss of transparent film is lost
Neden Analizi
Melt fracture is a manifestation of extrusion shear stress exceeding the critical value; die temperature too low or resin melt index too low both trigger it; the elastic melt of LDPE long branched chains is sensitive to this
Çözüm
① Raise the die temperature by 10-20℃; ② switch to high melt index resin; ③ add fluorinated elastomer processing aid PPA; after adjustment, take continuous samples to verify the effect, and resume mass production only after confirming stability
Temel Çıkarım
The essence of sharkskin is the shear critical; the three routes of raising die temperature, changing melt index, and adding PPA are selected according to cost; after confirming effectiveness, solidify the parameters and practices into the work instruction to prevent recurrence
LDPE;sharkskin;melt fracture;die temperature;PPA

Bu faydalı oldu mu?

0 kişi bunu faydalı buldu