Extrusion & Post
5 görüntüleme
LLDPE die gap
Sorun Belirtisi
LLDPE blown film produced per the LDPE die gap, bubble unstable and severe sharkskin.
Neden Analizi
LLDPE melt viscosity is high and shear-sensitive, requiring a larger die gap (0.060-0.100 inches) to reduce shear; During on-site troubleshooting, verify item by item according to this mechanism, avoiding blindly adjusting the machine based only on experience.
Çözüm
LLDPE die gap configured at 1.5-2.5mm; insufficient gap aggravates shear heat and melt fracture; After adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability.
Temel Çıkarım
LLDPE die gap must be larger than LDPE; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence; include this case in the defect archive as a reference for troubleshooting similar problems in the future.