Injection Molding
7 görüntüleme
PC Jetting Marks
Sorun Belirtisi
When the gate faces an open cavity, snake-shaped curved marks appear on the product surface, appearing as twisted stripes on transparent parts.
Neden Analizi
After the high-viscosity melt is ejected from the gate at high speed without hitting the wall, the melt strand folds and accumulates in the air; excessive initial injection speed and a small gate are the main causes.
Çözüm
①Change the gate angle so that the melt stream first hits the cavity wall; ②Reduce the initial injection speed and then speed up; ③Enlarge the gate; ④Increase the mold temperature.
Temel Çıkarım
Let the melt stream 'stick to the wall first and then spread out', and the jetting marks disappear.