PMMA Hot Runner Dead Corner Black Streaks

Sorun Belirtisi
Black streaks appear intermittently on transparent products, disappearing for a while after hot runner cleaning and then recurring.
Neden Analizi
Material accumulated in hot runner dead corners degrades slowly and periodically releases carbonized material forming black streaks; PMMA transparent parts are highly sensitive even to trace carbonized material.; During on-site troubleshooting, verify item by item according to this mechanism to avoid blindly adjusting the machine based on experience alone.
Çözüm
①Thoroughly clean the hot runner; ②evaluate dead-corner-free hot runner modification; ③shorten residence time; ④establish black streak cycle records.; After adjustment, continuously sample to verify the effect, and resume mass production only after confirming stability.
Temel Çıkarım
Intermittent black streaks point to hot runner stagnation; dedicated dead-corner-free hot runner systems are recommended for transparent parts.; After confirming effectiveness, fix the parameters and practices into the work instruction to prevent recurrence.
PMMA; hot runner; black streaks; dead corner; carbonization; cleaning