Injection Molding 6 görüntüleme

Severe EAA internal stress concentration

Sorun Belirtisi
EAA products with internal stress >15MPa causing cracking during storage
Neden Analizi
Injection speed too fast causing large orientation stress; uneven cooling freezing in thermal stress; improper gate position causing concentrated flow orientation
Çözüm
1) Reduce injection speed to reduce orientation; 2) Uniform mold temperature to reduce thermal stress; 3) Anneal at 80°C/4h to release stress; 4) Optimize gate position
Temel Çıkarım
Internal stress is caused by fast injection and uneven cooling; reducing speed, uniform cooling and annealing are key
EAAinternal stressorientation stressannealing treatmentuniform cooling