Extrusion & Post 11 görüntüleme

EAA vacuum section overflow

Sorun Belirtisi
Material overflow at the vacuum section of EAA extrusion, vent hole blocked
Neden Analizi
EAA melt viscosity low and overflowing at the vacuum section; vacuum section temperature too high making viscosity even lower and aggravating overflow; improper vent hole design
Çözüm
1) Reduce vacuum section temperature by 5-10°C to increase viscosity; 2) Add a baffle above the vent hole to prevent overflow; 3) Increase screw speed to accelerate conveying and reduce residence time
Temel Çıkarım
Overflow is caused by low melt viscosity; lowering temperature and adding a baffle is key
EAAvacuum section overflowmelt viscositytemperature reductionvent baffle