EMA vacuum vent overflow

Sorun Belirtisi
EMA extrusion vacuum section overflows, clogging the vent hole
Neden Analizi
EMA melt viscosity low, overflowing at the vacuum section; vacuum section temperature too high making viscosity even lower and worsening overflow; improper vent hole design
Çözüm
1) Lower vacuum section temperature by 5-10°C to increase viscosity; 2) Add baffle above the vent hole to prevent overflow; 3) Increase screw speed to accelerate conveying and reduce residence time
Temel Çıkarım
Overflow is caused by low melt viscosity; temperature reduction and baffle addition are key
EMA vacuum section overflow melt viscosity temperature reduction vent baffle